Our recommendation to fix white cabinets that have yellowed is to do a thorough sanding and precleaning and recoat with the following products:

GF advises extra care and prep when applying any finish over laminate surfaces because they are specifically designed not to mar and therefore they are not very "sand-able", making adherence difficult.

In addition to this non-permeable surface factor, General Finishes Gel Stain is an oil-based product, and it is more difficult to obtain proper drying characteristics over a dense manufactured surface such as laminate. Gel stains, as all wood stains, were formulated to go over raw wood which has an "open" surface and can absorb some of the stain.

Enduro-Var sprays beautifully if the gun is absolutely clean and does not have any other finish residue. Proper cleaning with acetone followed with hot water should purge the fluid passage. Enduro-Var itself will not cause gun failure.

Another possibility is the power of the gun. Some of the lower quality guns can overheat causing the product to cure in the gun - they need a rest once in a while if you are using them all day.

Also note that Enduro-Var ADHERES WELL only over WATER STAINS, DYE STAINS, and RAW WOOD.

If you want to change the sheen, you can re-coat with a different sheen over top. The second layer of top coat will replace the appearance of the first.

Sand lightly with a used 220 sanding PAD to knock down the original finish before re-coating. It may take two or 3 coats to get complete coverage.

Q: Which 12 colors will remain in the Milk Paint line?

You can rub down the finish with 0000 steel wool and General Finishes Orange Oil to lower the sheen.

Pro Tip: GF does not recommend using steel wool with water-based finishes because the particles can become embedded and rust.

Arm-R-Seal Blotching

The problem areas on your table are probably caused by surface contamination from oils, waxes or cleaning products used over the years.

Contaminants from dusting sprays that contain silicone will also impact the appearance and adherence of a finish - silicone is almost impossible to remove. Oil soaps and wax can also cause adhesion failures. This may be why the finish is performing differently on the leaves vs the table top. Adhesion failure is often more obvious in the deepest patterns of grain because the contamination is driven deep into the grain. 

Orange Peel while Spraying

One of the causes of orange peel is the application of too much fluid and not enough atomization to break the product up into smaller droplets. It's similar to putting your finger over the end of a garden hose. Increase the atomization by using smaller fluid tips or a larger spray unit. See General Finishes comparison chart for generally recommended spray tips. Contact your spray equipment manufacturer's recommendations as well.

General Finishes Arm-R-Seal

Although Arm-R-Seal rarely needs thinning because of its low viscosity, it can be thinned with up to 10% mineral spirits - more than that may thin the solids content too much.

Thinned Arm-R-Seal will be diluted but can be stored without risk of separation.